PERLINFO.gif (31823 bytes) Sponsored by INCON CORPORATION

SEARCH

Search explanation

See Also:

What is Perlite?

Home > Main Index > Markets > Construction Applications > Cement Plasters > Mix Proportions & Properties


Lightweight Fiber Reinforced Perlite Cement Plasters

Mix Design Data

The proper proportions of materials for various fiber reinforced perlite plasters are shown following table.

FIBER REINFORCED PERLITE PLASTER MIX PROPORTIONS & PROPERTIES

  Dry Density Average 28 Day Strength
      Compressive Flexural

Mix Proportions

lb/ft3 kg/m3 lb/in2 kPa lb/in 2 kPa
94 lbs (43 kg) Portland Cement (Type I/II)
50 lbs (23 kg) Lime (Type S)
6 ft3 (0.17 m3) Perlite Plaster Aggregate
4 lbs (2 kg) Alkali Resistant Glass Fibers
47 750 1000+ 6900+ 172 1186
94 lbs (43 kg) Portland Cement (Type I/II)
94 lbs Plastic Cement
6 ft3 (0.17 m3) Perlite Plaster Aggregate
1.4 lbs (0.6 kg) Polypropylene Fibers
46 740 1100+ 7600+ 164 1131
**
94 lbs (43 kg) Portland Cement (Type I/II)
94 lbs Plastic Cement
3 ft3 (0.085 m3) Perlite Plaster Aggregate
1.4 lbs (0.6 kg) Polypropylene Fibers
66 1050 1800+ 12,400+ 265 1830
94 lbs (43 kg) Portland Cement (Type I/II)
50 lbs (23 kg) Lime (Type S)
8 ft 3 (0.23 m3) Washed Plaster Sand
120 1920 1000+ 6900+ 167 1151

** high strength, high shear base fortile or veneer

Information given herein is from sources considered reliable, but no guarantee of accuracy can be made or liability assumed.  Your supplier may be able to provide you with more precise data.  Certain compositions or processes involving perlite may be the subject of patents.
Copyright © Incon Corporation 1996-2011.  All rights reserved.